UNS R30035
Typical Composition 0.025 max. C, 0.15 max. Mn, 0.015 max. P, 0.01 max. S, 0.15 max. Si, 19.00-21.00 Cr, 33.00-37.00 Ni, 9.00-11.00 Mo, 1.00 max. Ti, 0.01 B, 1.00 max Fe, Bal Co

Get the complete data sheet

Description Carpenter MP35N alloy is a nonmagnetic, nickel-cobalt-chromium-molybdenum alloy possessing a unique combination of ultrahigh tensile strength (up to 300 ksi [2068 MPa]), good ductility and toughness, and excellent corrosion resistance. In addition, this alloy displays exceptional resistance to sulfidation, high temperature oxidation, and hydrogen embrittlement.

The unique properties of MP35N alloy are developed through work hardening, phase transformation and aging. If the alloy is used in the fully work hardened condition, service temperatures up to 750°F (399°C) are suggested.
Applications Because of its unique combination of properties, MP35N alloy has been used in a wide variety of applications.

It has been used in fasteners, springs, nonmagnetic electrical components and instrument parts in medical, seawater, oil and gas well, and chemical and food processing environments.
Typical Room Temperature Tensile Properties % Cold Reduction Ultimate Tensile Strength 0.2% Yield Strength % Elongation % Reduction in Area Hardness
WORK STRENGTHENED
0 135 ksi (931 MPa) 60 ksi (414 MPa) 70 70 8 HRC
15 155 ksi (1069 MPa) 118 ksi (814 MPa) 41 70 29 HRC
25 170 ksi (1172 MPa) 150 ksi (1034 MPa) 28 65 34 HRC
35 194 ksi (1336 MPa) 154 ksi (1062 MPa) 22 67 42 HRC
45 228 ksi (1572 MPa) 189 ksi (1303 MPa) 17 62 47 HRC
55 265 ksi (1827 MPa) 205 ksi (1413 MPa) 12 50 47 HRC
65 280 ksi (1931 MPa) 235 ksi (1620 MPa) 11 49 50 HRC
WORK STRENGTHENED + AGED 1000 DEGREES F (538 C) 4 HRS., AIR COOLED
0 135 ksi (931 MPa) 60 ksi (414 MPa) 68 77 7 HRC
15 158 ksi (1089 MPa) 125 ksi (862 MPa) 39 70 33 HRC
25 186 ksi (1282 MPa) 175 ksi (1207 MPa) 24 65 39 HRC
35 203 ksi (1400 MPa) 195 ksi (1344 MPa) 21 62 43 HRC
45 257 ksi (1772 MPa) 251 ksi (1731 MPa) 12 52 46 HRC
53 300 ksi (2068 MPa) 290 ksi (1999 MPa) 10 48 50 HRC


Tensile Strength graph


Use our Technical Information database to get comprehensive technical data on hundreds of Carpenter alloys. The database is searchable and it's free.


U.S. locations that sell this product

International locations that sell this product



Terms of Site Use Privacy Statement email us
Copyright 1997-2008 CRS Holdings Inc.  All rights reserved.